Research article Topical Sections

Developments of pH responsive biodegradable monitoring film based on poly(vinyl alcohol) incorporated with Sappan heartwood extract for food packaging applications

  • The major problem leading to substantial waste in the food industry is the spoilage of food products during transportation and storage periods. Consequently, the scope of this research focuses on the development and preparation a pH responsive monitoring films based on biodegradable materials of poly(vinyl alcohol) (PVA) and natural colorant extract from Caesalpinia sappan L. heartwood (SP). These monitoring films were prepared by a solution casting method and the film stability was improved by crosslinking with citric acid (CA). The red tone of monitoring film without CA was observed, while the crosslinked monitoring film showed a yellow color, which occurs from the structural change of brazilin (structure presenting in SP) to brazilein under acidic conditions. From the SEM and FTIR results, the monitoring film showed high compatibility between phases, improvements in light barrier properties and good WVTR performance. The tensile strength and elongation at break were slightly increased. For pH responsive properties, the monitoring films showed a high response with NH3 gas detection with the change in color from a yellow tone to a red tone. These results indicated that the monitoring films have potential to be applied as food packaging for meat, fish, pork, chicken, and other foods that generate ammonium gas during spoilage. Therefore, these high stable, and non-toxic biodegradable PVA films that incorporated with SP extract and crosslinked by CA have the potential to be used for food spoilage detection in packaging.

    Citation: Worraphol Nansu, Gareth Ross, Sukunya Ross, Nungruthai Suphrom, Sararat Mahasaranon. Developments of pH responsive biodegradable monitoring film based on poly(vinyl alcohol) incorporated with Sappan heartwood extract for food packaging applications[J]. AIMS Materials Science, 2023, 10(3): 465-483. doi: 10.3934/matersci.2023026

    Related Papers:

    [1] Dorel Feldman . Poly(vinyl alcohol) nanocomposites: Recent contributions to engineering and medicine. AIMS Materials Science, 2021, 8(1): 119-129. doi: 10.3934/matersci.2021008
    [2] Chaitra Srikanth, Gattumane Motappa Madhu, Hemanth Bhamidipati, Siddarth Srinivas . The effect of CdO–ZnO nanoparticles addition on structural, electrical and mechanical properties of PVA films. AIMS Materials Science, 2019, 6(6): 1107-1123. doi: 10.3934/matersci.2019.6.1107
    [3] Lyudmyla V. Borkovska, Olexander Gudymenko, Olexander Stroyuk, Alexandra Raevskaya, Olena Fesenko, Tetyana Kryshtab . Photoinduced transformations of optical properties of CdSe and Ag-In-S nanocrystals embedded in the films of polyvinyl alcohol. AIMS Materials Science, 2016, 3(2): 658-668. doi: 10.3934/matersci.2016.2.658
    [4] Abdullah Ahmed Ali Ahmed, Abdullah Mohammed Al-Hussam, Abdu Mohammed Abdulwahab, Ahmed Nasser Ahmed Ali Ahmed . The impact of sodium chloride as dopant on optical and electrical properties of polyvinyl alcohol. AIMS Materials Science, 2018, 5(3): 533-542. doi: 10.3934/matersci.2018.3.533
    [5] Carlos A. Sánchez, Yamile Cardona-Maya, Andrés D. Morales, Juan S. Rudas, Cesar A. Isaza . Development and evaluation of polyvinyl alcohol films reinforced with carbon nanotubes and alumina for manufacturing hybrid metal matrix composites by the sandwich technique. AIMS Materials Science, 2021, 8(2): 149-165. doi: 10.3934/matersci.2021011
    [6] Rusul A. Ghazi, Khalidah H. Al-Mayalee, Ehssan Al-Bermany, Fouad Sh. Hashim, Abdul Kareem J. Albermany . Impact of polymer molecular weights and graphene nanosheets on fabricated PVA-PEG/GO nanocomposites: Morphology, sorption behavior and shielding application. AIMS Materials Science, 2022, 9(4): 584-603. doi: 10.3934/matersci.2022035
    [7] Mona Mohsen, Ehsan Gomaa, Nabila Ahmed Mazaid, Reem Mohammed . Synthesis and characterization of organic montmorillonite-polyvinyl alcohol-co-polyacrylic nanocomposite hydrogel for heavy metal uptake in water. AIMS Materials Science, 2017, 4(5): 1122-1139. doi: 10.3934/matersci.2017.5.1122
    [8] Nur Jassriatul Aida binti Jamaludin, Shanmugan Subramani . Thermal performance of LED fixed on CVD processed ZnO thin film on Al substrates at various O2 gas flow rates. AIMS Materials Science, 2018, 5(2): 246-256. doi: 10.3934/matersci.2018.2.246
    [9] Kanishka Jha, Ravinder Kataria, Jagesvar Verma, Swastik Pradhan . Potential biodegradable matrices and fiber treatment for green composites: A review. AIMS Materials Science, 2019, 6(1): 119-138. doi: 10.3934/matersci.2019.1.119
    [10] Shaimaa Mazhar Mahdi, Majeed Ali Habeeb . Low-cost piezoelectric sensors and gamma ray attenuation fabricated from novel polymeric nanocomposites. AIMS Materials Science, 2023, 10(2): 288-300. doi: 10.3934/matersci.2023015
  • The major problem leading to substantial waste in the food industry is the spoilage of food products during transportation and storage periods. Consequently, the scope of this research focuses on the development and preparation a pH responsive monitoring films based on biodegradable materials of poly(vinyl alcohol) (PVA) and natural colorant extract from Caesalpinia sappan L. heartwood (SP). These monitoring films were prepared by a solution casting method and the film stability was improved by crosslinking with citric acid (CA). The red tone of monitoring film without CA was observed, while the crosslinked monitoring film showed a yellow color, which occurs from the structural change of brazilin (structure presenting in SP) to brazilein under acidic conditions. From the SEM and FTIR results, the monitoring film showed high compatibility between phases, improvements in light barrier properties and good WVTR performance. The tensile strength and elongation at break were slightly increased. For pH responsive properties, the monitoring films showed a high response with NH3 gas detection with the change in color from a yellow tone to a red tone. These results indicated that the monitoring films have potential to be applied as food packaging for meat, fish, pork, chicken, and other foods that generate ammonium gas during spoilage. Therefore, these high stable, and non-toxic biodegradable PVA films that incorporated with SP extract and crosslinked by CA have the potential to be used for food spoilage detection in packaging.



    The freshness of a product while stored on a shelf is primarily determined by the quality of its fresh food components. Items such as meat, fish, pork, and chicken contain vital nutrients like protein, carbohydrates, fat, and vitamins. Unfortunately, these beneficial compounds can degrade or spoil over time, especially with extended storage [1,2,3]. Protein and high-fat products, in particular, have a shorter shelf life and tend to deteriorate more quickly. Generally, fresh food storage times are around 1–2 d at room temperature, 3–7 d below 4 ℃ (refrigeration) before deterioration, and around 1–3 months in the freezer. Several researchers have reported on the use of smart packaging for product protection, prevention, transportation, and indication [4,5].

    A method for evaluating the quality of food products is through the use of a food freshness indicator. This monitoring technique involves the preparation of intelligent film sensors, which are capable of detecting various factors affecting food freshness, such as temperature, time, humidity, oxygen levels, pH, microorganisms, and specific chemicals. These sensors are typically utilized in combination to provide accurate and comprehensive information about the freshness of a particular food product [6]. Of these factors pH-response is a popular and suitable technique for monitoring food freshness. As reported previously, the degradation of protein and fat in food products can lead to the generation of volatile nitrogen, which can serve as a source of bacteria. Additionally, the spoilage of food items such as meat, pork, chicken, and seafood can result in changes to their color and composition, as noted in studies [7,8,9]. Numerous studies have focused on the development of intelligent film indicators using biodegradable polymers, such as chitin-chitosan [10], starch [3,11], wheat protein [12,13] cellulose and its derivative [14,15], also poly(vinyl alcohol) (PVA) [16,17,18,19,20].

    PVA is a biodegradable and commercial polymer that finds widespread use in various applications among other biodegradable polyesters, such as poly(lactic acid), polycaprolactone, poly(butylene succinate) [21,22,23,24,25]. The use is including medical, cosmetic, and food products, due to its non-toxic, biodegradable, biocompatible, and water-soluble properties [26,27,28]. However, PVA also exhibits limitations in terms of its properties such as mechanical, barrier, thermal and heat stability. An important factor in the responsiveness of intelligent films is the use of sensitive dyes and pigments. Typically, synthetic dyes such as methyl red, cresol red, bromocresol green, bromocresol purple, chlorophenol, bromine thymol blue, and xylenol are incorporated as pH-responsive color sensors [1,29,30]. However, the toxicity of synthetic dyes has raised concerns about contamination in food and other products. As a result, many researchers have focused on developing eco-friendly dyes and replacing synthetic dyes with natural alternatives [2,5,13,19,31,32].

    Natural dyes can be derived from various sources, including minerals, animals, vegetables, fruits, and plants. Plant-based natural dyes are typically obtained from various plant parts such as the bark, flower, leaf, root, peel, and fruit, which are rich in polyphenolic compounds and responsive compounds such as flavonoids and anthocyanins [1,2,30,31,32,33]. Caesalpinia sappan L., also known as Sappan wood, is a traditional medicinal plant in the Leguminosae family. Its heartwood has been used in various applications, including cosmetics, food and beverage, medical, and coloring [3,34,35,36]. The heartwood of Sappan (Caesalpinia sappan L.) exhibits an orange-red color after extraction with either water or an ethanolic solvent. It has been found to contain a high concentration of polyphenolic compounds, with the main chemical constituent being brazilin. Brazilin appears orange in color and undergoes a chemical structure change to brazilein, which turns the color to red [37,38].

    The use of Sappan heartwood extract in pH-responsive research is less common compared to anthocyanins, which undergo a broad spectrum of color transformations. The heartwood of the Sappan tree has been utilized in the development and integration of packaging films for various purposes, such as those used in meat packaging [3], food sensors [38]. This is due to its ability to effectively absorb UV light and its responsiveness to changes in pH. Therefore, this study aims to create a monitoring film that can respond to changes in pH, suitable for use in fresh food applications. The film is made using poly(vinyl alcohol) (PVA) and sappan heartwood extract (SP), and its stability is ensured by incorporating citric acid (CA) as a crosslinking agent. The biodegradable monitoring film is prepared using the solution casting method for film formation. The physicochemical properties of the monitoring film, including film appearance, color index, morphology, water vapor transmission rate (WVTR), mechanical properties, and pH-responsiveness, are observed and reported in this study.

    Commercial grade poly(vinyl alcohol) (PVA) powder was purchased from Ajax Finechem Pty Ltd, with molecular weight of 30,000–50,000 Da. Citric acid (food grade) was used the crosslinking agent. Sappan heartwood (SP) was purchased from Niyom Osot, a local medicinal plant shop located in Phitsanulok province, Thailand. Glycerol was used as a plasticizing agent supplied by Fisher chemical company. 30% NH3 ammonia solution (AR/ACS) was purchased from LOBA CHEMIE PVT.Ltd.

    Dried Sappan heartwood (SP) was chopped into small pieces with sizes of 5 mm × 80 mm. 50 g of SP were immersed into 300 mL of 80%v/v ethanol (weight ratio of 1:6) and kept at room temperature for 72 h without exposure to light. After that, the SP heartwood was subsequently removed from the ethanolic solution by Whatman filter paper No 40. The obtained solution was evaporated at a temperature of 50 ℃ using rotating evaporator (100 rpm). After completion, 2 g of crude ethanolic SP extract was dissolved in 95% ethanol and the concentration was adjusted to 20 %w/v before use [39].

    7.5 g PVA powders were dissolved in 100 mL de-ionized water before addition of 20 %wt of glycerol. The solution was heated in a water bath with the applied temperature of 60 ℃ and continuously stirred for 3 h. The 20 %w/v SP extracts at 0.1, 0.2 and 0.3 %wt were then added into the mixture of PVA. Different concentrations of citric acid (crosslinking agent) at 0, 2, 4, 6, 8 and 10 %wt were loaded into the mixture of PVA and SP extracts, and continuously stirred for 30 min. After that, 20 mL of mixture was poured into silicon molds with dimensions of 3 cm × 15 cm. The film thickness was controlled by the volume of solution and measured by digital micrometer. The resultant film was then dried in laboratory hood at room temperature for 24 h and kept in zip lock plastic bags for 2 d before testing. The films from PVA and PVA incorporated with SP extracts were labeled as PVA, 0.1SP, 0.2SP, 0.3SP. Whereas, films crosslinked by CA were labeled first using the concentration of SP extract followed by the concentration of CA, for example, 0.1SP+2CA, 0.2SP+6CA, 0.3 SP+10CA.

    The color index of the films was measured by a color reader CR-20 via computer data analysis. The films were measured at 5 points per sample and the data was shown in term of lightness (L), redness (a) and yellowness (b). The color difference (ΔE) was calculated by Eq 1 [39].

    ΔE=[(LL2)+(aa2)+(bb2)] (1)

    UV-Vis light absorption was characterized by the UV-Vis spectroscopy (SPECORD 200 PLUS model). Wavelength covered the UV and visible regions (200–800 nm). The films were cut to a square shape of 2.0 cm × 2.0 cm before testing. The opacity of films was measured by the UV-vis and used Eq 2, where Abs600 is an absorbance of film at 600 nm [40].

    Opacity=Abs600Thicknessoffilm(mm) (2)

    Morphology of the films was characterized by scanning electron microscope (SEM) (LeO1455VP model). The sample was cut into a square shape and fixed on to the SEM stub sample holder with double-side adhesive carbon tape before being coated by the gold and tested.

    The water vapor transmission rate (WVTR) was measured following previous work and ASTM E96 [41] (gravimetric method). Briefly, the films were cut into a square shape of 2.0 cm × 2.0 cm and average film thickness of 0.3 mm. The films then covered a centrifuge tube (volume of 15 mL) that contained 10.00 g of dried desiccant. Afterward, they were kept in a desiccator at room temperature with a humidity of 50%. The weight change in the films was monitored every 24 h for 168 h, with WVTR values calculated following Eq 3 [42].

    WVTR=ΔWATimes (3)

    Where, ∆W is the weight change (g), A is a film area (mm2) and Time is the tested date (day).

    Chemical functional group of the films was characterized by Fourier transform infrared (ATR-FTIR) technique (model Spectrum GX, Perkin Elmer). SP extracts and films were dried in a hot air oven at 45 ℃ for 24 h before FTIR testing. The wavenumber measurement was collected at Mid-IR wavelengths (4,000–400 cm−1) at room temperature.

    Mechanical properties of films were tested using a universal tensile testing machine (Instron 5965), following the ASTM D882 procedure. Films were cut into a square shape of 1.00 cm × 5.00 cm and the film thickness was measured by digital vernier calipers. The tensile test method used a cross ahead speed of 40 mm/min, load force of 0.1 kN and gauge length of 20.00 mm. The film samples were prepared with 5 specimens per sample. The data was calculated with average value and standard deviation (SD) of tensile strength at break (TS), %elongation at break (EB) and tensile modulus (TM).

    NH3 response was tested by a modified head space detection method [43]. 30% NH3 solution was diluted to 10 %v/v and 5 mL of the solution was added in a glass container. Film samples were cut into square shapes sized 2.00 cm2 and then stuck to the inside of the lid of glass container. The container was then closed with the sample containing lid and left at room temperature at 55% humidity. NH3 detection was measured by monitoring the change of the film color at different times of 0, 5, 10, 15, 20, 30 and 60 min. Optical photographs were taken to observe the film's color change by mobile phone (iPhone 11) 2× magnification.

    The color of the produced biodegradable monitoring films were measured and reported as the color parameter index: lightness (L), redness (a), yellowness (b), and total color difference (∆E) (Table 1). Pure PVA film color index depicted high lightness, high transparency and no color change, while PVA films incorporated with SP extracts at 0.1, 0.2, and 0.3 %wt exhibited a decrease in lightness value and an increase in redness (a) and yellowness (b) values, which were influenced by the brazilein content of SP extract. Generally, the natural colors of brazilin and brazilein ranges from yellow to red color, and they are capable of undergoing a chemical transformation when the conditions are changed [44]. PVA films with 0.1, 0.2 and 0.3 %wt SP extract and crosslinking agent at 2, 4, 6, 8 and 10 %wt showed the color parameter index slightly shifted to yellow due to the film becoming more acidic. The L value of monitoring films crosslinked by CA showed an increase in transparency when compared with PVA film without CA. Similarly, the redness (a) and yellowness (b) values of films increased when higher amount of CA were added. Under acidic conditions, the chemical structure of brazilein is converted into the brazilin structure, which in turn is the underlying reason for the differences in color parameter. Moreover, total color difference (∆E) of films with SP extract and CA showed much higher values than pure PVA film.

    Table 1.  Color parameter index of biodegradable monitoring film from PVA and SP extracts.
    Sample L (Lightness) a (green-red) b (blue-yellow) ∆E
    7.5PVA 86.98 ± 0.41 −0.48 ± 0.04 −3.36 ± 0.18 Ref
    0.1SP 41.70 ± 2.99 47.18 ± 1.47 40.24 ± 2.09 78.88
    0.1SP + 2CA 30.48 ± 0.64 46.58 ± 1.44 26.72 ± 1.65 79.45
    0.1SP + 4CA 36.88 ± 1.57 54.24 ± 2.54 36.14 ± 4.79 84.05
    0.1SP + 6CA 72.30 ± 2.38 22.12 ± 1.65 91.36 ± 4.72 98.48
    0.1SP + 8CA 72.28 ± 0.72 24.10 ± 1.11 88.46 ± 2.29 96.18
    0.1SP + 10CA 76.72 ± 1.75 11.94 ± 1.98 76.46 ± 4.49 81.43
    0.2SP 77.02 ± 0.33 13.06 ± 0.38 77.96 ± 0.61 83.04
    0.2SP + 2CA 72.80 ± 1.69 23.66 ± 2.21 95.18 ± 3.15 102.44
    0.2SP + 4CA 68.82 ± 0.92 27.22 ± 0.88 83.28 ± 3.05 92.76
    0.2SP + 6CA 71.92 ± 0.71 24.54 ± 1.38 87.80 ± 1.87 95.72
    0.2SP + 8CA 71.90 ± 0.66 22.34 ± 1.07 90.10 ± 2.89 97.38
    0.2SP + 10CA 70.08 ± 1.57 26.74 ± 2.63 82.98 ± 5.78 92.09
    0.3SP 70.46 ± 0.80 27.58 ± 1.77 87.94 ± 4.66 96.93
    0.3SP + 2CA 65.10 ± 1.34 32.68 ± 1.71 73.60 ± 4.32 86.61
    0.3SP + 4CA 67.00 ± 1.32 30.58 ± 1.59 78.24 ± 5.20 89.57
    0.3SP + 6CA 64.70 ± 0.83 29.46 ± 0.96 83.10 ± 8.76 94.17
    0.3SP + 8CA 66.98 ± 0.89 26.56 ± 0.32 90.92 ± 2.95 100.10
    0.3SP + 10CA 69.26 ± 1.62 26.32 ± 1.78 89.54 ± 3.91 98.30

     | Show Table
    DownLoad: CSV

    The UV-Vis light absorption of the biodegradable monitoring films is observed in Figure 1. The PVA films incorporated with SP extract at 0.1, 0.2 and 0.3 %wt exhibited two absorption peaks at 458 nm and 550 nm (Figure 1a). These absorption peaks corresponded to the absorption of chemical structures of brazilin (458 nm) and brazilein (550 nm), which are the natural pigments presented in SP extract [44]. However, the absorbance intensity depended on the amount of brazilin contents in monitoring film, in which higher SP contents promoted higher absorbance intensity. The PVA films incorporated with SP extracts and CA at different concentrations were also observed (Figure 1bd). The absorption peak was observed at 454 nm, which was an absorption peak from the chemical structure of brazilin. The disappearance of absorption peak from brazilein (at approximately 550 nm) is due to the deprotonation of the brazilein chromophore to brazilin under acidic conditions when crosslinking with CA [44,45].

    Figure 1.  UV-vis light absorbance of biodegradable monitoring films: (a) PVA and PVA incorporated with 0.1, 0.2 and 0.3 %wt of SP extract, (b) PVA incorporated with 0.1 %wt SP extract with CA, (c) PVA incorporated with 0.2 %wt SP extract with CA and (d) PVA incorporated with 0.3 %wt SP extract with CA. For (b, c and d), different concentrations of CA were used at 2, 4, 6, 8 and 10 %wt.

    The opacities of biodegradable monitoring films were reported by dividing the absorbance of films at 600 nm (A600) by film thickness (Figure 2). The PVA film incorporated with SP extracts showed higher opacity (lower transparency) than that of pure PVA. The increase in opacity was observed when higher content of SP extract was applied to the film. However, a decrease in opacity (increase in transparency) was observed when CA was added into the high SP content films. The concentrations of CA did not significant effect the opacity of the monitoring films.

    Figure 2.  Opacity of biodegradable PVA and monitoring films with different concentrations of SP extracts (0.1, 0.2 and 0.3 %wt) and citric acid (0, 2, 4, 6, 8 and 10 %wt).

    The surface morphology of the monitoring films with different SP extracts were observed in Figure 3 by SEM at 500× magnification. PVA film without SP extract showed a smooth surface, while PVA films incorporated with SP extracts at 0.1, 0.2 and 0.3 %wt showed small particles distributed within the PVA matrixes with different electron densities, in which higher amounts of SF extracts (white phase) exhibited higher numbers of particles with bigger sizes due to particle agglomeration.

    Figure 3.  SEM images of PVA film (a), and biodegradable monitoring films at 0.1 %wt SP (b), 0.2 %wt SP (c), and 0.3 %wt SP (d), at magnification of 500×.

    Figure 4 shows the measurement of the water vapor transmission rate (WVTR) using a gravimetric method, which is a crucial physical property of films utilized in the food industry. PVA films with and without SP extracts (0.1–0.3 %wt) showed similar values of WVTR with all films showing an increase in WVTR with longer testing times (Figure 4a). However, films incorporated with SP extracts (especially at 0.1 %wt) seems to have slightly lower WVTR values than the pure PVA film. Generally, WVTR of films is affected by many factors such as nature of the barrier (polymer, crystallinity, homogeneity, molecular weight, hydrophilicity, etc.), film structure (homogeneous, multilayer, etc.), and thermodynamics (temperature, vapor pressure, physical state of water in contact to the films, etc.). In this case of PVA and SP extracts, there is possible formation of strong hydrogen bonding between hydroxyl groups of PVA and brazilin that cause changes in film structure to behave as a better barrier to water (lower in WVTR value) than pure PVA. This result was similar to the previous reported research, which prepared active films mixed with natural active compounds that are the rich source of polyphenolic compounds [46,47].

    Figure 4.  Water vapor transmission rate (WVTR) of biodegradable monitoring films with different tested time (a) PVA film and PVA mixed with SP extracts, (b) 0.1%wt SP with CA, (c) 0.2%wt SP with CA, and (d) 0.3%wt SP with CA.

    The WVTR values of the biodegradable monitoring films with different concentrations of SP extracts (0.1, 0.2 and 0.3 %wt) and CA (2, 4, 6, 8 and 10 %wt) were also studied (Figure 4bd). These films showed a significant decrease in WVTR values when compared to the PVA and PVA incorporated with SP extracts (Figure 4a). For 0.1 %wt SP extract (Figure 4b), there was a decrease in WVTR values with higher contents of CA. For 0.2 and 0.3 %wt SP extract (Figure 4c, d, respectively), the changes in WVTR were similar when different concentrations of CA were used. The reason for the dramatical decrease in WVTR values of the monitoring films of PVA incorporated with SP extracts and crosslinked with CA was similar to the results from PVA and SP extracts but there is more influence from greater strong hydrogen bonding, and crosslinked structures (prohibiting the alignment of PVA chains). In addition, this would be effect to the hydrophilicity of films, therefore, the measurement of contact angle of films was necessary.

    Hydrophilicity of biodegradable monitoring films was measured by contact angle and the results are presented in Figure 5. Pure PVA film showed the highest surface contact angle (approximately 90º), which proved the films are hydrophilic. After incorporation of SP extract, the films showed lower contact angles, demonstrating the increase in hydrophilicity (more hydrophilic) (Figure 5a). All films of PVA incorporated with different concentrations of SP extracts and CA (Figure 5bd) showed contact angle values lower than PVA film and PVA films incorporated with SP extracts (without CA). However, at high concentrations of CA seems to affect to the hydrophilicity of films, as the excess CA molecules (a high-water surface absorption and solubility) are possible to migrate to the surface of film and then enhanced the increase of contact angle (more hydrophobic).

    Figure 5.  Hydrophilicity of biodegradable monitoring films: (a) PVA and PVA incorporated with 0.1, 0.2 and 0.3 %wt of SP extract, (b) PVA incorporated with 0.1 %wt SP extract with CA, (c) PVA incorporated with 0.2 %wt SP extract with CA and (d) PVA incorporated with 0.3 %wt SP extract with CA. For (b, c and d), different concentrations of CA were used at 2, 4, 6, 8 and 10 %wt.

    ATR-FTIR spectra of biodegradable monitoring films based on PVA incorporated with SP extract and crosslinked by citric acid was observed and compared with pure PVA and pure SP extracts (Figure 6). The frequency broad bands of PVA film was observed at 3270 cm−1, which attributed to the –OH stretching and hydrogen bonded. Peak at 2918 cm−1 was the C–H stretching on the PVA backbone. The strong vibration peak at 1713 cm−1 attributed to C = O of vinyl acetate and 1246 cm−1 related to the C–O bending of alcohol functional group of PVA. The SP extract showed characteristic peaks at 3250 cm−1 (–OH stretching and hydrogen bonded) and 2900–2800 cm−1 (CH3, CH2 stretching). Peaks at 1606 cm−1, 1466 cm−1 and 1085 cm−1 were attributed to C = C stretching of brazilin backbone, C–H bending, and C-O stretching vibration, respectively. Films of PVA incorporated with different concentrations of SP extracts (0.1SP, 0.2SP and 0.3 SP) showed the same characteristic peaks of PVA and SP extracts. A small shift of the peaks at 1713 cm−1 (C = O stretching of vinyl acetate) and 1085 cm−1 (C–O stretching) was observed when compared PVA incorporated SP extracts with pure PVA and SP extract. The monitoring film crosslinked by citric acid showed the characteristic peaks of PVA and SP extract with the frequency shift of peaks at 1713 cm−1 and a broader band of –OH stretching and hydrogen bonded at 3270 cm−1. The reason for the frequency shift and a broader band was due to the formation of ester linkage intermolecular forces that was formed by hydrogen bonding in these films [48]. This causes a change in the electron cloud that alters the resonant frequency of that particular bond to have slightly different hydrogen bonding states leading to different frequencies and a broad band [49].

    Figure 6.  ATR-FTIR spectra of biodegradable monitoring films of PVA, SP extract, PVA incorporated with SP extracts at 0.1, 0.2 and 0.3 %wt SP and PVA incorporated with SP extract and citric acid.

    Mechanical properties of the biodegradable monitoring films were observed by tensile testing and the results were reported as tensile strength (TS), %elongation at break (EB), and tensile modulus (TM). From Figure 7a, tensile strength of pure PVA film had a TS at 24.20 MPa, after the addition of SP extract at 0.1 %wt and 0.3 %wt there was a very small increase in TS at 28.76 and 24.66 MPa, respectively. However, a decrease in TS of film at 0.2 %wt SP extract (19.68 MPa) was observed when compared with pure PVA, which might be due to the effect of plasticizing behavior of SP extract. This can be confirmed by %elongation at break (Figure 7b). %Elongation at break of pure PVA film is depicted at 255.20%, while that of PVA film incorporated with 0.1, 0.2, and 0.3 %wt SP extract showed at 591.80,648.00, and 613.20% respectively. In addition, the tensile modulus of all films was significantly lower than pure PVA film (Figure 7c). One possible explanation of the increase in %elongation at break and decrease in tensile modulus of films was due to the plasticizing effect interaction generated between the hydroxyl group of glycerol, brazilin and the PVA polymer chains. This results in a greater flexibility of the polymer chains, allowing for the increase in polymer chain's mobility and improved overall flexibility of the polymer materials. The previous research work reported chemical structures that are rich-polyphenol compounds to act as plasticizing agent and improve the film mechanical properties [50]. Tensile strength, %Elongation at break and tensile modulus of all these films were slightly affected by the concentrations of SP extracts and CA, therefore the optimum concentrations should be considered depending on the require application.

    Figure 7.  Tensile properties of biodegradable monitoring films (a) tensile strength at break (TS), (b) %Elongation at break (EB), and (c) tensile modulus (TM).

    pH responsive is a main factor in films used for food spoilage detection. The color response of the biodegradable monitoring films was observed when exposed to ammonia (NH3). The volatile NH3 was detected by the monitoring film as a color change which is shown schematically in Figure 8a. Figure 8b showed the chemical structure change of brazilin to brazilein under oxidation, which changes color from yellow (brazilin) to red (brazilein). The monitoring film based on PVA was reacted with citric acid and brazilin in SP extract. The hydroxyl group of PVA reacted with carbonyl group of citric acid and hydroxyl group of brazilin (Figure 8c) [38,51].

    Figure 8.  Cartoon schematic of monitoring film before and after pH response, chemical structure change of brazilin to brazilein, and possible chemical structure of film fabricated from PVA, SP extract and CA.

    The pH response was detected at different detection times and the results are shown in Figure 9. Monitoring films incorporated with SP extract showed an orange to red color depending on the SP extract concentration before NH3 detection. After 5 min detection time, the color of monitoring film is slightly shifted from the orange-red color to dark red because of the brazilin structure hydrogen deprotonation [36,51].

    Figure 9.  pH response of biodegradable monitoring film incorporated with 0.1 %wt, 0.2 %wt, and 0.3 %wt SP extract (captured by iPhone 11 at 2×).

    Figure 10 depicts the pH-responsive monitoring films at 0.1 %wt SP–0.3 %wt SP extract content and crosslinked with 2–10 %wt CA. The monitoring film color shows a yellow color before NH3 detection. After NH3 detection the color shifts from a yellow color to the orange and then dark red as the exposure time increases from 5 to 60 min. Furthermore, the color response of 0.2 %wt and 0.3 %wt SP extract withs different CA concentrations are shown in Figure 10b, c, respectively. These results show the same trend as the non-crosslinked films with a yellow color before detection and after detection the color changes to orange and dark red. The high concentration of crosslinking agent influences the color response and detection due to the acidic medium inhibited the deprotonating on the brazilin chemical structure [51]. However, high concentrations of SP extract improved the real-time detection and high crosslinking agent concentrations improved the film stability. Thus, these results enable the films to monitor food spoilage with NH3 sensitive detection. Moreover, the monitoring film shows high stability with water contact more than 7 d without microbial contamination and showed more than 3 months stability at room temperature and atmospheric conditions.

    Figure 10.  pH response of biodegradable monitoring film incorporated with SP extract crosslinked by CA at 2–10 %wt (a) 0.1 %wt SP, (b) 0.2 %wtSP, and (c) 0.3%wt SP (captured by iPhone 11 at 2×).

    A biodegradable monitoring film based on polyvinyl alcohol (PVA) was developed by incorporating sappan heartwood extract (SP) as a food deterioration indicator. The film's stability was improved through crosslinking with citric acid (CA). SP extract contains brazilin, a key chemical compound that undergoes color changes upon chemical structure transformation. The physical properties of the monitoring film, including color parameters, water vapor transmission rate (WVTR), light transmission, and light absorption, as well as its morphology, hydrophilicity, chemical structure, tensile strength, and flexibility, were investigated using techniques such as scanning electron microscopy, contact angle measurement, FTIR-ATR, and tensile testing. The film's pH responsiveness was also evaluated through headspace NH3 volatile detection. The research results showed that the incorporation of SP extract improved the optical properties of the monitoring film, including enhanced UV light absorption and reduced WVTR values, which could be attributed to the strong hydrogen bonding interactions between SP extract and the polymer's side chains. Additionally, the film's stability was improved through crosslinking with CA, as evidenced by the mechanical property results. The pH responsiveness of the film was demonstrated through real-time color changes from yellow to dark red upon NH3 volatile detection. Specifically, the film incorporating 0.2 %wt SP extract and crosslinked with CA at 4–8 %wt exhibited favorable properties in terms of optical properties, stability, and pH responsiveness, making it suitable for food freshness detection while ensuring non-toxicity to customers. Overall, the biodegradable monitoring film developed in this study shows great potential for effective detection of fresh food spoilage and could be applied in food packaging applications to ensure food quality and safety.

    The authors declare they have not used Artificial Intelligence (AI) tools in the creation of this article.

    This work was supported by Naresuan University (NU), and National Science, Research and Innovation Fund (NSRF), Grant Number R2565B078 and was partially supported by Global and Frontier Research University, Grant Number R2566C052, Naresuan University and the European Union's Horizon 2020 research and innovation programme under the Marie Sklodowska-Curie grant agreement No 871650 (MEDIPOL). Also, thanks to the Science Lab Centre, Faculty of Science, Naresuan University for support.

    The authors declare that there is no conflict of interest regarding the publication of this manuscript.



    [1] Cheng H, Xu H, McClements DJ, et al. (2022) Recent advances in intelligent food packaging materials: Principles, preparation and applications. Food Chem 375: 131738. https://doi.org/10.1016/j.foodchem.2021.131738 doi: 10.1016/j.foodchem.2021.131738
    [2] Almasi H, Forghani S, Moradi M (2022) Recent advances on intelligent food freshness indicators; an update on natural colorants and methods of preparation. Food Packag Shelf Life 32: 100839. https://doi.org/10.1016/j.fpsl.2022.100839 doi: 10.1016/j.fpsl.2022.100839
    [3] Khumkomgool A, Saneluksana T, Harnkarnsujarit N (2020) Active meat packaging from thermoplastic cassava starch containing sappan and cinnamon herbal extracts via LLDPE blown-film extrusion. Food Packag Shelf Life 26: 100557. https://doi.org/10.1016/j.fpsl.2020.100557 doi: 10.1016/j.fpsl.2020.100557
    [4] Hong LG, Yuhana NY, Zawawi EZE (2021) Review of bioplastics as food packaging materials. AIMS Mater Sci 8: 166–184. https://doi.org/10.3934/matersci.2021012 doi: 10.3934/matersci.2021012
    [5] Hashim SB, Tahir HE, Liu L, et al. (2022) Intelligent colorimetric pH sensoring packaging films based on sugarcane wax/agar integrated with butterfly pea flower extract for optical tracking of shrimp freshness. Food Chem 373: 131514. https://doi.org/10.1016/j.foodchem.2021.131514 doi: 10.1016/j.foodchem.2021.131514
    [6] Janjarasskul T, Suppakul P (2018) Active and intelligent packaging: The indication of quality and safety. Crit Rev Food Sci Nutr 58: 808–831. https://doi.org/10.1080/10408398.2016.1225278 doi: 10.1080/10408398.2016.1225278
    [7] Domínguez R, Barba FJ, Gómez B, et al. (2018) Active packaging films with natural antioxidants to be used in meat industry: A review. Food Res Int 113: 93–101. https://doi.org/10.1016/j.foodres.2018.06.073 doi: 10.1016/j.foodres.2018.06.073
    [8] Wang Q, Jiang Y, Chen W, et al. (2022) Development of pH-responsive active packaging materials based on purple corncob and its application in meat freshness monitoring. Food Res Int 161: 111832. https://doi.org/10.1016/j.foodres.2022.111832 doi: 10.1016/j.foodres.2022.111832
    [9] Chayavanich K, Thiraphibundet P, Imyim A (2020) Biocompatible film sensors containing red radish extract for meat spoilage observation. Spectrochim Acta-Part A Mol Biomol Spectrosc 226: 117601. https://doi.org/10.1016/j.saa.2019.117601 doi: 10.1016/j.saa.2019.117601
    [10] Gao HX, He Z, Sun Q, et al. (2019) A functional polysaccharide film forming by pectin, chitosan, and tea polyphenols. Carbohydrate Polymer 215: 1–7. https://doi.org/10.1016/j.carbpol.2019.03.029 doi: 10.1016/j.carbpol.2019.03.029
    [11] Khalid S, Yu L, Feng M, et al. (2018) Development and characterization of biodegradable antimicrobial packaging films based on polycaprolactone, starch and pomegranate rind hybrids. Food Packag Shelf Life 18: 71–79. https://doi.org/10.1016/j.fpsl.2018.08.008 doi: 10.1016/j.fpsl.2018.08.008
    [12] Moradi M, Kousheh SA, Razavi R, et al. (2021) Review of microbiological methods for testing protein and carbohydrate-based antimicrobial food packaging. Trends Food Sci Technol 111: 595–609. https://doi.org/10.1016/j.tifs.2021.03.007 doi: 10.1016/j.tifs.2021.03.007
    [13] Zhang X, Zou W, Xia M, et al. (2022) Intelligent colorimetric film incorporated with anthocyanins-loaded ovalbumin-propylene glycol alginate nanocomplexes as a stable pH indicator of monitoring pork freshness. Food Chem 368: 130825. https://doi.org/10.1016/j.foodchem.2021.130825 doi: 10.1016/j.foodchem.2021.130825
    [14] Vargas-Torrico MF, von Borries-Medrano E, Aguilar-Méndez MA (2022) Development of gelatin/carboxymethylcellulose active films containing Hass avocado peel extract and their application as a packaging for the preservation of berries. Int J Biol Macromol 206: 1012–1025. https://doi.org/10.1016/j.ijbiomac.2022.03.101 doi: 10.1016/j.ijbiomac.2022.03.101
    [15] Thennakoon TM, Ching YC, Chuah CH, et al. (2020) pH-responsive poly(lactic acid)/sodium carboxymethyl cellulose film for enhanced delivery of curcumin in vitro. J Drug Deliv Sci Technol 58: 101787. https://doi.org/10.1016/j.jddst.2020.101787 doi: 10.1016/j.jddst.2020.101787
    [16] Koosha M, Hamedi S (2019) Intelligent Chitosan/PVA nanocomposite films containing black carrot anthocyanin and bentonite nanoclays with improved mechanical, thermal and antibacterial properties. Prog Org Coatings 127: 338–347. https://doi.org/10.1016/j.porgcoat.2018.11.028 doi: 10.1016/j.porgcoat.2018.11.028
    [17] Andrade J, González-Martínez C, Chiralt A (2022) Antimicrobial PLA-PVA multilayer films containing phenolic compounds. Food Chem 375: 131861. https://doi.org/10.1016/j.foodchem.2021.131861 doi: 10.1016/j.foodchem.2021.131861
    [18] Yao X, Liu J, Hu H, et al. (2022) Development and comparison of different polysaccharide/PVA-based active/intelligent packaging films containing red pitaya betacyanins. Food Hydrocoll 124: 107305. https://doi.org/10.1016/j.foodhyd.2021.107305 doi: 10.1016/j.foodhyd.2021.107305
    [19] Lin X, Li N, Xiao Q, et al. (2022) Polyvinyl alcohol/starch-based film incorporated with grape skin anthocyanins and metal-organic framework crystals for colorimetric monitoring of pork freshness. Food Chem 395: 133613. https://doi.org/10.1016/j.foodchem.2022.133613 doi: 10.1016/j.foodchem.2022.133613
    [20] Z. Miao, R. Lv, S. Teng, et al. (2022) Development of antioxidant active packaging films with slow release properties incorporated with tea polyphenols-loaded porous starch microcapsules. Int J Biol Macromol 222: 403–412. https://doi.org/10.1016/j.ijbiomac.2022.09.143 doi: 10.1016/j.ijbiomac.2022.09.143
    [21] Ross GM, Ross S, Tighe BJ (2017) Chapter 23-Bioplastics: New routes, new products, In: Gilbert M, Brydson's Plastics Materials, 8th Eds., Oxford: Butterworth Heinemann, 631–652. https://doi.org/10.1016/B978-0-323-35824-8.00023-2
    [22] Ross S, Topham PD, Tighe BJ (2013) Identification of optically clear, miscible regions of ternary polymer blends using a novel rapid screening method. Polym Int 66: 44–51. https://doi.org/10.1002/pi.4512 doi: 10.1002/pi.4512
    [23] Suaduang N, Ross S, Ros GM, et al. (2019) The physical and mechanical properties of biocomposite films composed of poly(lactic acid) with spent coffee grounds. Key Eng Mater 824: 1662–9795. https://doi.org/10.4028/www.scientific.net/KEM.824.87 doi: 10.4028/www.scientific.net/KEM.824.87
    [24] Tuancharoensri N, Ross GM, Kongprayoon A, et al. (2023) In situ compatibilized blends of PLA/PCL/CAB melt-blown films with high elongation: Investigation of miscibility, morphology, crystallinity and modelling. Polymers 15: 303. https://doi.org/10.3390/polym15020303 doi: 10.3390/polym15020303
    [25] Kongprayoon A, Ross G, Limpeanchob N, et al. (2022) Bio-derived and biocompatible poly(lactic acid)/silk sericin nanogels and their incorporation within poly(lactide-co-glycolide) electrospun nanofibers. Polym Chem 13: 3343–3357. https://doi.org/10.1039/D2PY00330A doi: 10.1039/D2PY00330A
    [26] Tuancharoensri N, Ross G, Punyodom W, et al. (2022) Multifunctional core-shell electrospun nanofibrous fabrics of poly(vinyl alcohol)/silk sericin (core) and poly(lactide-co-glycolide) (shell). Polym Int 71: 266–275. https://doi.org/10.1002/pi.6319 doi: 10.1002/pi.6319
    [27] Kumkun P, Tuancharoensri N, Ross G, et al. (2019) Green fabrication route of robust, biodegradable silk sericin and poly(vinyl alcohol) electrospun nanofibrous scaffolds. Polym Int 68: 1903–1913. https://doi.org/10.1002/pi.5900 doi: 10.1002/pi.5900
    [28] Sonjan S, Ross GM, Mahasaranon S, et al. (2021) Biodegradable hydrophilic film of crosslinked PVA/silk sericin for seed coating: The effect of crosslinker loading and polymer concentration. J Polym Environ 29: 323–334. https://doi.org/10.1007/s10924-020-01867-9 doi: 10.1007/s10924-020-01867-9
    [29] Shao P, Liu L, Yu J, et al. (2021) An overview of intelligent freshness indicator packaging for food quality and safety monitoring. Trends Food Sci Technol 118: 285–296. https://doi.org/10.1016/j.tifs.2021.10.012 doi: 10.1016/j.tifs.2021.10.012
    [30] Wang Y, Zhang J, Zhang L (2022) An active and pH-responsive film developed by sodium carboxymethyl cellulose/polyvinyl alcohol doped with rose anthocyanin extracts. Food Chem 373: 131367. https://doi.org/10.1016/j.foodchem.2021.131367 doi: 10.1016/j.foodchem.2021.131367
    [31] Roy S, Rhim JW (2021) Anthocyanin food colorant and its application in pH-responsive color change indicator films. Crit Rev Food Sci Nutr 61: 2297–2325. https://doi.org/10.1080/10408398.2020.1776211 doi: 10.1080/10408398.2020.1776211
    [32] Zeng P, Chen X, Qin YR, et al. (2019) Preparation and characterization of a novel colorimetric indicator film based on gelatin/polyvinyl alcohol incorporating mulberry anthocyanin extracts for monitoring fish freshness. Food Res Int 126: 108604. https://doi.org/10.1016/j.foodres.2019.108604 doi: 10.1016/j.foodres.2019.108604
    [33] Shah MA, Bosco SJD, Mir SA (2014) Plant extracts as natural antioxidants in meat and meat products. Meat Sci 98: 21–33. https://doi.org/10.1016/j.meatsci.2014.03.020 doi: 10.1016/j.meatsci.2014.03.020
    [34] Sirirak J, Suppharatthanya P, Chantha K, et al. (2021) Eco-friendly lake pigment from sappanwood: Adsorption study and its application as natural colorant for natural rubber toy balloon. J Met Mater Miner 31: 27–37. https://doi.org/10.55713/jmmm.v31i2.1009 doi: 10.55713/jmmm.v31i2.1009
    [35] Patanathabutr P, Hongsriphan N (2021) Sappan natural dyed biocomposites from poly(Lactic acid) and aluminum silicate synthesized via sol-gel method from rice husk ash. Eng J 25: 305–315. https://doi.org/10.4186/ej.2021.25.2.305 doi: 10.4186/ej.2021.25.2.305
    [36] Rina O, Ibrahim S, Dharma A, et al. (2017) Stabilities natural colorant of Sappan wood (Caesalpinia sappan L.) for food and beverages in various pH, temperature, and matrices of food. Int J Chem Tech Res 10: 98–103.
    [37] Nirmal NP, Rajput MS, Prasad RGSV, et al. (2015) Brazilin from Caesalpinia sappan heartwood and its pharmacological activities: A review. Asian Pac J Trop Med 8: 421–430. https://doi.org/10.1016/j.apjtm.2015.05.014 doi: 10.1016/j.apjtm.2015.05.014
    [38] Romruen O, Kaewprachu P, Karbowiak T, et al. (2022) Development of intelligent gelatin films incorporated with Sappan (Caesalpinia sappan L.) heartwood extract. Polymers-Basel 14: 1–14. https://doi.org/10.3390/polym14122487 doi: 10.3390/polym14122487
    [39] Nansu W, Chaiwut P, Ross S, et al. (2021) Developments of biodegradable polymer based on polylactic acid (PLA) with natural color extracts for packaging film applications. J Met Mater Miner 31: 127–133. https://doi.org/10.55713/jmmm.v31i3.1147 doi: 10.55713/jmmm.v31i3.1147
    [40] Cheng M, Kong R, Zhang R, et al. (2021) Effect of glyoxal concentration on the properties of corn starch/poly(vinyl alcohol)/carvacrol nanoemulsion active films. Ind Crops Prod 171: 113864. https://doi.org/10.1016/j.indcrop.2021.113864 doi: 10.1016/j.indcrop.2021.113864
    [41] ASTM International (1995) Standard test methods for water vapor transmission of materials. ASTM E 96.
    [42] Sobhan A, Muthukumarappan K, Wei L (2022) A biopolymer-based pH indicator film for visually monitoring beef and fish spoilage. Food Biosci 46: 101523. https://doi.org/10.1016/j.fbio.2021.101523 doi: 10.1016/j.fbio.2021.101523
    [43] Liang T, Sun G, Cao L, et al. (2019) A pH and NH3 sensing intelligent film based on Artemisia sphaerocephala Krasch. gum and red cabbage anthocyanins anchored by carboxymethyl cellulose sodium added as a host complex. Food Hydrocoll 87: 858–868. https://doi.org/10.1016/j.foodhyd.2018.08.028 doi: 10.1016/j.foodhyd.2018.08.028
    [44] Ngamwonglumlert L, Devahastin S (2023) Brazilein as an alternative pigment: Isolation, characterization, stability enhancement and food applications. Food Chem 398: 133898. https://doi.org/10.1016/j.foodchem.2022.133898 doi: 10.1016/j.foodchem.2022.133898
    [45] Ngamwonglumlert L, Devahastin S, Chiewchan N, et al. (2020) Color and molecular structure alterations of brazilein extracted from Caesalpinia sappan L. under different pH and heating conditions. Sci Rep 10: 1–10. https://doi.org/10.1038/s41598-020-69189-3 doi: 10.1038/s41598-020-69189-3
    [46] Dong H, Ling Z, Zhang X, et al. (2020) Smart colorimetric sensing films with high mechanical strength and hydrophobic properties for visual monitoring of shrimp and pork freshness. Sensors Actuators B Chem 309: 127752. https://doi.org/10.1016/j.snb.2020.127752 doi: 10.1016/j.snb.2020.127752
    [47] Chatkitanan T, Harnkarnsujarit N (2020) Development of nitrite compounded starch-based films to improve color and quality of vacuum-packaged pork. Food Packag Shelf Life 25: 100521. https://doi.org/10.1016/j.fpsl.2020.100521 doi: 10.1016/j.fpsl.2020.100521
    [48] de Lima GG, Ferreira BD, Matos M, et al. (2020) Effect of cellulose size-concentration on the structure of polyvinyl alcohol hydrogels. Carbohydr Polym 245: 116612. https://doi.org/10.1016/j.carbpol.2020.116612 doi: 10.1016/j.carbpol.2020.116612
    [49] Yooyod M, Ross GM, Limpeanchob N, et al. (2016) Investigation of silk sericin conformational structure for fabrication into porous scaffolds with poly(vinyl alcohol) for skin tissue reconstruction. Eur Polym J 81: 43–52. https://doi.org/10.1016/j.eurpolymj.2016.05.023 doi: 10.1016/j.eurpolymj.2016.05.023
    [50] Wu LT, Tsai IL, Ho YC, et al. (2021) Active and intelligent gellan gum-based packaging films for controlling anthocyanins release and monitoring food freshness. Carbohydr Polym 254: 117410. https://doi.org/10.1016/j.carbpol.2020.117410 doi: 10.1016/j.carbpol.2020.117410
    [51] Ngamwonglumlert L, Devahastin S, Chiewchan N, et al. (2020) Color and molecular structure alterations of brazilein extracted from Caesalpinia sappan L. under different pH and heating conditions. Sci Rep 10: 1–10. https://doi.org/10.1038/s41598-020-69189-3 doi: 10.1038/s41598-020-69189-3
  • This article has been cited by:

    1. Heba Isawi, Emad M. Ahmed, Marwa Rabee, Hesham Moustafa, Using natural antioxidant Rhubarb extracts in PVA/chitosan bio-adsorbent films for efficient removal of cationic and anionic dyes from polluted water, 2024, 1226086X, 10.1016/j.jiec.2024.09.049
    2. Pranav P. Ajith, Omar Bashir, Kulwinder Kaur, Tawheed Amin, Rafeeya Shams, Kshirod Kumar Dash, Sappan wood extraction for intelligent gelatin packaging films: a review on implementing green packaging solutions, 2024, 81, 0170-0839, 15349, 10.1007/s00289-024-05444-1
  • Reader Comments
  • © 2023 the Author(s), licensee AIMS Press. This is an open access article distributed under the terms of the Creative Commons Attribution License (http://creativecommons.org/licenses/by/4.0)
通讯作者: 陈斌, bchen63@163.com
  • 1. 

    沈阳化工大学材料科学与工程学院 沈阳 110142

  1. 本站搜索
  2. 百度学术搜索
  3. 万方数据库搜索
  4. CNKI搜索

Metrics

Article views(2638) PDF downloads(162) Cited by(2)

Figures and Tables